Elder Lab Staining Airborne Microplastics

Elder Lab Staining Airborne Microplastics

Materials

Biological Safety Cabinet (BSC)

Side arm flask, 150-1000 mL

Small pin Fritted glass filter

Vacuum and tubing

0.5 µm Sepcon Filters

1.7 mL microcentrifuge tubes

Microcentrifuge

ddH2O (Barnstead 18 MΩ)

100% isopropanol (IPA)

100% Ethanol (EtOH)

70% Ethanol (EtOH)

0.4% Gibco Trypan Blue (TB) – 1 year shelf life

99.99% MCE Nile Red (NR) Powder

20 µL and 1 mL pipettors

Amber Glass vials for stain storage

250°C Oven

Gloves (nitrile)

Parafilm

100% Cotton Lab Coat -No Plastic Fibers

SiMPore Filters with nano/microparticles

Tweezers cleaned with IPA to manipulate the SiMPore filter from container to the fritted glass filter

Lionheart Plate Reader – Ben Miller Lab

All glassware is to be cleaned per SOP MP-4 Glass and Reagent Preparation

 

 

 

Procedure

  1. Sample Collection

See “GilanSamplingRev1_2.docx” for sampling procedure

 

  1. Stain Preparation

Wash hands and put on lab coat and gloves. Within the BSC, spray everything with 70% EtOH and wipe using Kimwipes. Nile red is prepared by mixing ~50 mg in 45 mL of 100% EtOH in a centrifuge tube. About 10 uL of this is diluted with EtOH to 1µg/mL to yield 10 mL, thoroughly vortexing ~30s before and after adding the 10 uL. Depending on the initial mass dispensed, calculate the remaining volume needed from the stock tube to dilute the second tube to achieve 1 µg/mL. In an amber glass vial, add 1 mL of 1 µg/mL NR, then dilute with 4 mL of ddH2O. Into an amber glass vial cleaned per SOP MP-4, use a Sepcon to filter the 5 mL of working concentration NR (0.2 ug/mL), and keep up to 30 days.

 

Example:

50 mg NR Powder/45mL EtOH = 1.111 µg/mL

(x mL)(1.111 µg/mL) = (10 mL)(1 µg/mL)

X mL = 0.009 mL = 9 µL

 

(9 uL)(1.111 µg/mL NR) + (9.991 mL EtOH) = 1 µg/mL in EtOH

(1 mL)( 1 µg/mL NR) + (4mL Sepcon filtered ddH2O) = 0.2 µg/mL NR in 20% EtOH

 

Cf = 0.2 µg/mL

Vf = 10 mL

 

4 mL of commercially prepared 0.4% Trypan Blue from Gibco is diluted to 0.04% in 0.9% Saline and centrifuged through a Sepcon filter into an amber vial.

 

  1. Staining Procedure

Wash hands and put on lab coat and gloves. Within the BSC, spray everything with at least 70% EtOH and wipe using Kimwipes. Remove the parafilm sealing the glass Petri dish containing the SiMPore filter using tweezers. Place the filter on the fritted glass filter facing up and the troughs pointing down. You can identify the bottom by how the filter is seated in the plastic housing unit. Do not touch the filter with the pipette tip. Try using your other hand as a fulcrum to reduce motion.

For Nile Red, apply 60 µL in 10 µL increments in a sweeping motion across each of the 3 windows with the vacuum on (20 uL per window). The vacuum is left of for at least 1 minute to let dry before turning off and returning the filter to its Petri dish for imaging.

If desired, apply a 20 µL drop of 0.04% Trypan Blue to the filter and let soak ~1 min after staining with NR. Turn on the vacuum and wash 2 times with 250 µL of ddH2O being careful not to let water touch the black disc and fall through filter. After the washes are completed, turn off the vacuum.

 

 

 

  1. Imaging

See SOP “Using the Nikon Epifluorescent Microscope in Goergen Hall B109” OR “SOP Lionheart FX Microscope – Rm 5-5144.docx”

 

  1. Clean up

Put the vacuum tube away. Disassemble the side arm flask and fritted glass filter and wash with Dawn/Green Clean/ etc. Rinse glassware with tap water followed by a 2-5% Alconox rinse. Rinse 3 times with 0.22 µm Barnstead ddH2O and fill with IPA. Sonicate the pieces for 3-5 minutes and cap the pieces with aluminum foil as they are pulled out of the sonicator and bake in oven at 250°C for 6-12 hours. Reassemble the pieces and cover with aluminum until next use.

 

  1. Interpretation

See SOP “Image J Airborne MPs” and “Lionheart Meta Data”. Blue stained objects are cellulosic, e.g. cotton. Nile Red positive objects are very likely to be plastics, but composition needs to be confirmed by other specific techniques.

 

 